Hydrogen attack of steel. Progress report, April 1, 1978--March 31, 1979
Description:
Four normalized carbon steels made in different ways (Si-killed, Al-killed, REM-treated, and electroslag refined) were studied to determine the role of differing fine inclusions on the early stages of hydrogen attack (HA). Hydrogen exposures were made at 450/sup 0/C (6.5 MPa) and 375/sup 0/C (7.6 MPa). The first stage of HA is shown to be the development of a closely spaced (1-2 ..mu..m) array of small bubbles over the ferrite/pearlite, or occasionally the ferrite/ferrite boundaries. These grew…
more
Date:
December 27, 1978
Creator:
Shewmon, P. G.
Partner: