CORROSION ANALYSIS: LOW-CAPACITY PUMP. Large Sodium Pump Study, Phase II. Page: 26 of 30

io
0Y
r10-10
M.
E
LU
C.)
U
C.)
LU
Cn10_12
LL 0.8
U-
W
C)
W~ 0
x

200

300

400

500

600

TEMPERATURE (0C)
Figure 8 Wear Rates and Friction Coefficients for Stellite I and Stellite 3 in Sodium
3117-8

20

S SITE I
- STELLITE I-STELLITE I
S STELL ITE 3-STELL ITE 3 10, ()
(2) STELLITE 6-STELLITE I
0 2 kg
- 4 4-5 kg _
- -
I I II

Upcoming Pages

Here’s what’s next.

upcoming item: 27 27 of 30
upcoming item: 28 28 of 30
upcoming item: 29 29 of 30
upcoming item: 30 30 of 30

Show all pages in this report.

This report can be searched. Note: Results may vary based on the legibility of text within the document.

Tools / Downloads

Get a copy of this page .

Citing and Sharing

Basic information for referencing this web page. We also provide extended guidance on usage rights, references, copying or embedding.

Reference the current page of this Report.

Thomas, K.C. & Shiels, S. CORROSION ANALYSIS: LOW-CAPACITY PUMP. Large Sodium Pump Study, Phase II., report, October 31, 1970; Madison, Pennsylvania. (https://digital.library.unt.edu/ark:/67531/metadc1034653/m1/26/ocr/: accessed April 24, 2019), University of North Texas Libraries, Digital Library, https://digital.library.unt.edu; crediting UNT Libraries Government Documents Department.

International Image Interoperability Framework (This Page)